Material Standard

ASTM A479 Download

ASTM A479/A479M is the ASTM International specification for stainless steel bars and shapes intended for use in boilers and other pressure vessels, and for general applications requiring corrosion resistance. The companion ASME SA-479 adopts identical requirements for ASME BPVC compliance. HT PIPE stocks A479 bars in all major grades with full traceability and Mill Test Certificates per EN 10204 3.1.

1. Standard Scope & Designation

ASTM A479 covers hot-rolled or cold-finished stainless steel bars and shapes in straight lengths:

Form Typical Sizes Finish
Round Bar 6–330 mm diameter Hot-rolled, T&P, cold-drawn
Square Bar 6–200 mm Hot-rolled, cold-finished
Hexagon Bar 8–100 mm AF Cold-drawn, cold-finished
Flat Bar Width 10–200 mm; t 3–50 mm Hot-rolled, cold-rolled
Scope Statement (ASTM A479-23): "This specification covers stainless steel bars and shapes for use in boilers and other pressure vessels and for general application purposes."
Designation Issuing Body Unit System Latest Edition
ASTM A479 ASTM International Inch-Pound A479-23
ASTM A479M ASTM International SI (Metric) A479M-23
ASME SA-479 ASME (BPVC Sec. II Part A) Both 2023 Edition

2. Stainless Steel Grades Covered

2.1 Austenitic Grades

Grade UNS No. Key Feature Typical Applications
304 / 304L S30400 / S30403 18Cr-8Ni / Low C Pressure vessels, tanks, piping
316 / 316L S31600 / S31603 16Cr-10Ni-2Mo Marine, chemical, pharma
321 / 321H S32100 / S32109 Ti-stabilized; high-temp Exhaust, turbine, aerospace
347 / 347H S34700 / S34709 Nb-stabilized; high-temp Pressure vessels, high-temp piping
310S / 309S S31008 / S30908 25Cr-20Ni / 22Cr-12Ni heat resisting Furnace parts, heat exchangers

2.2 Ferritic & Martensitic Grades

Grade UNS No. Type Typical Applications
410 S41000 Martensitic Turbine blades, valve parts, shafts
416 / 416Se S41600 / S41623 Martensitic (free-machining) Automatic screw machine parts
420 S42000 Martensitic Surgical instruments, cutlery
440A / 440C S44002 / S44004 Martensitic (high-C) Bearings, valves, surgical tools
430 / 430F S43000 / S43020 Ferritic / Ferritic (free-mach.) Decorative, nitric acid service

2.3 Duplex Grades

Grade UNS No. PREN Typical Applications
2205 S31803 / S32205 ~35 Oil & gas, chemical process
F53 / F55 S32750 / S32760 40–43 Offshore, seawater, subsea

Full grade listing per ASTM A479-23 Tables 1–6. Free-machining grades 303 (S30300), 416 (S41600), 430F (S43020), 440F (S44020) are also listed.

3. Chemical Composition — Key Grades (ASTM A479 Table 1)

Values are maximum unless shown as a range. Product analysis tolerances per ASTM A480/A480M.

Grade C % Mn % Si % P % S % Cr % Ni % Mo % N % Other
304 0.07 2.00 0.75 0.045 0.030 17.5–19.0 8.0–10.5 0.10
304L 0.030 2.00 0.75 0.045 0.030 17.5–19.0 8.0–12.0 0.10
316 0.07 2.00 0.75 0.045 0.030 16.0–18.0 10.0–14.0 2.0–3.0 0.10
316L 0.030 2.00 0.75 0.045 0.030 16.0–18.0 10.0–14.0 2.0–3.0 0.10
321 0.08 2.00 0.75 0.045 0.030 17.0–19.0 9.0–12.0 0.10 Ti: 5×C–0.70
347 0.08 2.00 0.75 0.045 0.030 17.0–19.0 9.0–13.0 Nb+Ta: 10×C–1.00
410 0.15 1.00 1.00 0.040 0.030 11.5–13.5 0.75
430 0.12 1.00 1.00 0.040 0.030 16.0–18.0 0.75
2205 0.030 2.00 1.00 0.030 0.020 22.0–23.0 4.5–6.5 3.0–3.5 0.14–0.20

Note: Free-machining grades (303, 416, 430F) have S up to 0.15–0.35%. Martensitic 440A/440C have C up to 0.60–1.20%. Full tables in ASTM A479-23.

4. Mechanical Property Requirements (ASTM A479 Table 2)

Minimum requirements in the required heat-treated condition. Elongation gauge: 4D for round bar specimens.

Grade UNS Tensile Strength min
MPa (ksi)
Yield Strength 0.2%
min MPa (ksi)
Elongation
min %
Hardness max
304 S30400 515 (75) 205 (30) 30 201 HB / 92 HRB
304L S30403 485 (70) 170 (25) 30 201 HB / 92 HRB
316 S31600 515 (75) 205 (30) 30 217 HB / 95 HRB
316L S31603 485 (70) 170 (25) 30 217 HB / 95 HRB
321 S32100 515 (75) 205 (30) 30 217 HB / 95 HRB
347 S34700 515 (75) 205 (30) 30 217 HB / 95 HRB
310S S31008 515 (75) 205 (30) 30 217 HB / 95 HRB
410 S41000 450 (65) 205 (30) 20 217 HB / 96 HRB
430 S43000 450 (65) 205 (30) 22 183 HB / 89 HRB
2205 S32205 620 (90) 450 (65) 25 293 HB / 31 HRC

Martensitic grades in hardened & tempered condition have different requirements. Hardness for martensitic 410: max 217 HB in annealed condition; up to 40 HRC in hardened & tempered condition.

5. Heat Treatment Requirements

Grade Family Required Condition Heat Treatment Cooling
Austenitic (304, 316, 321, 347…) Solution Annealed 1010–1120°C (1850–2050°F) Rapid quench — water or air
Ferritic (430…) Annealed 760–900°C (1400–1650°F) Air cool or water quench
Martensitic (410, 420…) Annealed or H&T Anneal: 750–900°C; Harden: 925–1010°C; Temper: per type Air/oil quench; subsequent temper
Duplex (2205…) Solution Annealed 1020–1100°C (1870–2010°F) Rapid water quench

6. Testing & Inspection Requirements

Test Requirement Reference
Chemical Analysis (Heat) One per heat; all elements per grade table ASTM A479 Tables 1–6
Tensile Test One per lot; longitudinal bar specimen (4D gauge) ASTM A370
Hardness Test Mandatory on each end of each bar ASTM E10 / E18
Intergranular Corrosion Supplementary — "L" grades and stabilized grades ASTM A262 Practice A or E
Intermetallic Phase (Duplex) Supplementary — duplex grades ASTM A923 Method A, B, or C

7. Dimensions & Tolerances

Product Size Range Tolerance Standard Typical Length
Hot-Rolled Round Bar 13–330 mm dia. ASTM A484/A484M 3–6 m random
Cold-Finished Round Bar 6–100 mm dia. ASTM A484/A484M (CF) 3–6 m / exact length
Square & Hexagon Bar 6–200 mm ASTM A484/A484M 3–6 m random
Flat Bar Width 10–200 mm; t 3–50 mm ASTM A484/A484M 3–6 m random

Hot-rolled round bar: ±0.5 mm for 25–50 mm dia.; ±1.0 mm for 50–100 mm dia. Cold-finished bars: h9–h11 tolerances (much tighter). Full tables in ASTM A484/A484M.

8. Industries & Applications

Industry Recommended Grades Typical Components
Boilers & Pressure Vessels 304, 304L, 316L, 321, 347 Flanges, staybolts, nozzle internals
Oil & Gas 316L, 2205, 410 Valve stems, pump shafts, wellhead parts
Chemical Processing 316L, 904L, 2205, 2507 Mixer shafts, agitator parts
Food & Beverage 304L, 316L Shafts, pump impellers, mixers
Fasteners & Hardware 303, 416, 410, 430F Bolts, nuts, screws (free-machining)
Medical & Surgical 420, 440C, 304 Surgical instruments, implants

9. ASTM A479 vs ASTM A276 — Key Differences

Criteria ASTM A479 ASTM A276
Primary Application Boilers and pressure vessels General engineering
Heat Treatment Solution annealing mandatory; documented Annealed, hot-finished, or cold-drawn
Hardness Verification Mandatory on each end of each bar Per lot only
Marking Heat no., grade, ASTM A479, HT lot Heat no., grade, ASTM A276
ASME BPVC Adopted as ASME SA-479 (Sec. II Part A) Not adopted by ASME
Selection Tip: For ASME Code-stamped pressure vessels, use ASME SA-479. For general mechanical engineering (shafts, fasteners, hardware), ASTM A276 is more economical. Always consult the governing code for your specific application.

10. Related Standards

Standard Scope Relationship
ASTM A276 Stainless Steel Bars and Shapes (general) General-purpose alternative to A479
ASTM A484/A484M General Requirements for Stainless Steel Bars Dimensional & tolerance standard
ASTM A370 Mechanical Testing of Steel Products Tensile, hardness test methods
ASTM A262 Sensitization / IGC Testing Supplementary requirement for A479
ASME SA-479 ASME BPVC Section II Part A ASME adoption for Code work

11. How to Order — Required Information

No. Item Requirement / Example
1 Specification ASTM A479 or ASME SA-479
2 Grade / Type e.g., Type 304 (UNS S30400)
3 Product Form Round, square, hexagon, flat bar
4 Size / Dimensions e.g., Round 50 mm dia. × 3 m
5 Finish / Condition Hot-rolled; T&P; cold-drawn; solution annealed
6 Supplementary Tests A262 IGC, A923 intermetallic, UT
7 Certification EN 10204 3.1 CMTR
8 Quantity Weight (kg / metric ton)
Download ASTM A479 / A479M Standard (PDF)

Go to Download Center  |  Request MTC / Quotation

12. Frequently Asked Questions

Q: What is ASTM A479 stainless steel bar used for?

ASTM A479 bars are used inside boilers and pressure vessels (staybolts, flange ring segments, nozzle internals, baffles), for general corrosion-resistant mechanical applications (shafts, pump parts, valve stems), and for machined components in the food, pharmaceutical, chemical, oil & gas, and medical industries.

Q: What is the difference between ASTM A479 and ASTM A276?

ASTM A479 is written for pressure vessel bars with mandatory end hardness testing on each bar, mandatory documented solution annealing, and mandatory lot traceability. ASTM A276 is a general-purpose bar specification without these requirements. A479 is adopted by ASME as SA-479; A276 is not part of ASME BPVC.

Q: What are the mechanical properties of ASTM A479 Type 316L?

Type 316L (UNS S31603): minimum tensile strength 485 MPa (70 ksi), yield strength 0.2% offset min. 170 MPa (25 ksi), elongation min. 30% in 4D gauge length, hardness max. 217 HB / 95 HRB, in solution-annealed condition.

Q: Is ASTM A479 Type 316L bar suitable for marine applications?

Yes — Type 316L provides substantially better chloride corrosion resistance than 304L due to its 2–3% molybdenum addition, making it suitable for marine atmospheres, coastal environments, and light seawater exposure. For highly aggressive seawater or subsea applications, duplex 2205 (PREN ~35) or super-duplex 2507/255 (PREN 40+) are recommended.

Q: What diameter ranges are available for ASTM A479 bars?

Hot-rolled rounds: 13–330 mm diameter. Cold-finished rounds (tighter tolerances, better surface finish): 6–100 mm diameter. Squares: 6–200 mm. Hexagons: 8–100 mm AF (across flats). Length: typically 3–6 m random; exact cut lengths available on request.

Q: Can ASTM A479 bars be used in ASME Code stamped equipment?

Yes — when ordered to ASME SA-479 (the ASME BPVC Section II Part A adoption of ASTM A479). The material must be accompanied by Certified Material Test Reports (CMTR) documenting chemical composition, heat treatment, and mechanical properties, and is subject to authorized inspector review for Code-stamped assemblies.

Request a Quote — ASTM A479 Stainless Steel Bars & Shapes

HT PIPE stocks and supplies ASTM A479 / ASME SA-479 stainless steel bars in all major grades (304, 316, 321, 347, 410, 2205 and more), in rounds, squares, hexagons, and flat bars. EN 10204 3.1 CMTRs included.