news
ASTM B473 Standard for nickel alloy bar and wire
Chemical Requirements | |||
Element | UNS N08026 | UNS N08020 | UNS N08024 |
C max | 0.03 | 0.07 | 0.03 |
Mn,max | 1 | 2 | 1 |
P,max | 0.03 | 0.046 | 0.035 |
S, max | 0.03 | 0.035 | 0.035 |
Si,max | 0.5 | 1 | 0.5 |
Ni | 33.00 to 37.20 | 32.00 to 38.00 | 35.00-40.00 |
Cr | 22.00 to 26.00 | 19.00 to 21.00 | 22.50 to 25.00 |
Mo | 5.00 to 6.70 | 2.00 to 3.00 | 3.50 to 5.00 |
Cu | 2.00 to 4.00 | 3.00 to 4.00 | 0.50 to 1.50 |
Nb+Ta | ... | 8*carbon-1.00 | 0.15 to 0.35 |
N | 0.10 to 0.16 | ... | ... |
Fe | remainder | remainder | remainder |
Mechanical Property Requirements | |||||||||
Condition | Diameter or thickness,in(mm) | Tensile Strength, min | Yield Strength, min | Elongation in 2 in.(50.8mm), min,% | Reduction of area, min, % | ||||
ksi | MPa | ksi | MPa | ||||||
Annealed, hot finished or cold finished | All | 80 | 551 | 35 | 241 | 30.8 | 50 | ||
Annealed, stran-hardened | Up to 2(50.8)incl | 90 | 620 | 60 | 415 | 15 | 40 |